| Material | Spec / condition | ρ kg/m³ | E GPa | Sy MPa | Sut MPa | Se MPa | Corrosion / UV | $/kg | Uses and notes |
|---|---|---|---|---|---|---|---|---|---|
| AISI 1045 steel aisi-1045-cd Carbon & alloy steels | ASTM A108 / SAE J403 cold drawn | 7,850 | 205 | 530 | 630 | — | poor ≤ 400 °C | 1.2–2.5 | shafts, pins, keys, couplings |
| AISI 4140 alloy steel aisi-4140-qt Carbon & alloy steels | ASTM A322 / A434 quenched & tempered (≈ HRC 28–32) | 7,850 | 205 | 655 | 965 | — | poor ≤ 425 °C | 2–4 | highly loaded shafts, gears, high-strength bolts |
| AISI 4340 alloy steel aisi-4340-qt Carbon & alloy steels | ASTM A322 / AMS 6415 quenched & tempered 540 °C | 7,850 | 205 | 1,080 | 1,170 | — | poor ≤ 425 °C | 3–6 | main shafts, heavy gears |
| AISI 8620 steel, carburised aisi-8620-carb Carbon & alloy steels | SAE J404 / AGMA 2001 Grade 2 case carburised, core ≈ HRC 30–35 | 7,850 | 205 | 830 | 1,100 | — | poor | 2.5–5 | gears, pinions AGMA allowable bending ≈ 380–450 MPa, contact ≈ 1240–1550 MPa (Grade 1–2) |
| ASTM A36 structural steel astm-a36 Carbon & alloy steels | ASTM A36 hot rolled | 7,850 | 200 | 250 | 400 | — | poor / excellent | 0.9–1.6 | plates, base plates, brackets, frames Minimum specified values: Fy 250 MPa, Fu 400–550 MPa |
| ASTM A572 Grade 50 astm-a572-50 Carbon & alloy steels | ASTM A572 hot rolled | 7,850 | 200 | 345 | 450 | — | poor | 1–1.8 | tower sections, frames, plates |
| ASTM A500 Grade C round tube (HSS) astm-a500-c Carbon & alloy steels | ASTM A500 cold formed | 7,850 | 200 | 317 | 427 | — | poor | 1.2–2.2 | towers, masts, hollow shafts (low speed) Round HSS Fy = 46 ksi; AISC 360 design thickness 0.93 × nominal |
| Stainless steel 304 ss-304 Stainless steels | ASTM A240 / A276 annealed | 8,000 | 193 | 215 | 505 | — | good / excellent ≤ 870 °C | 3–6 | fasteners, enclosures, fittings |
| Stainless steel 316 ss-316 Stainless steels | ASTM A240 / A276 annealed | 8,000 | 193 | 205 | 515 | — | excellent / excellent | 4–8 | marine/coastal hardware, fasteners A4 |
| 17-4 PH stainless ss-17-4ph Stainless steels | ASTM A564 H1150 | 7,800 | 197 | 725 | 930 | — | good | 8–15 | corrosion-resistant shafts, pins |
| Aluminium 6061-T6 al-6061-t6 Aluminium alloys | ASTM B221 / B209 T6 | 2,700 | 68.9 | 276 | 310 | 96.5 | good / excellent ≤ 150 °C | 3–6 | frames, blade spars (small), housings, solar racking Fatigue strength at 5×10⁸ cycles (no endurance limit); welding reduces strength in the HAZ to ≈ 50 % |
| Aluminium 6063-T6 al-6063-t6 Aluminium alloys | ASTM B221 T6 | 2,700 | 68.9 | 214 | 241 | — | good / excellent | 3–5 | extrusions, solar module frames, racking rails |
| Aluminium 5083-H116 (marine) al-5083-h116 Aluminium alloys | ASTM B928 H116 | 2,660 | 70.3 | 215 | 305 | — | excellent / excellent | 4–7 | marine structures, welded frames |
| Ductile iron 65-45-12 di-65-45-12 Cast irons | ASTM A536 as cast | 7,100 | 169 | 310 | 448 | — | fair | 1.5–3 | gearbox housings, hubs, bearing housings |
| Grey iron Class 30 gi-class-30 Cast irons | ASTM A48 as cast | 7,200 | 100 | — | 214 | — | fair | 1–2.5 | housings, brake discs, machine bases (damping) Brittle; compressive strength ≈ 750 MPa |
| Bearing bronze C93200 (SAE 660) bronze-c93200 Copper alloys | ASTM B505 continuous cast | 8,930 | 100 | 125 | 240 | — | good | 9–15 | plain bearings, bushings, thrust washers |
| Copper C11000 (ETP) cu-c11000 Copper alloys | ASTM B152 / B187 half hard | 8,890 | 117 | 250 | 290 | — | good | 9–13 | windings, bus bars, earthing |
| Titanium Ti-6Al-4V ti-6al-4v Titanium | ASTM B348 / AMS 4928 annealed | 4,430 | 113.8 | 880 | 950 | 510 | excellent | 25–60 | weight-critical highly stressed parts |
| NdFeB magnet N42 ndfeb-n42 Magnetic materials | IEC 60404-8-1 / maker grade sintered, Ni-Cu-Ni coated | 7,500 | — | — | 80 | — | poor / good ≤ 80 °C | 50–120 | PM generators, magnetic clutch actuation, magnetic couplings Br ≈ 1.28–1.32 T; irreversible loss above max temperature (use N42SH for 150 °C); brittle; coat against corrosion |
| Ferrite magnet C8 (Y30) ferrite-c8 Magnetic materials | IEC 60404-8-1 sintered | 4,900 | — | — | — | — | excellent ≤ 250 °C | 2–5 | low-cost PM generators, holding magnets Br ≈ 0.38–0.40 T; loses strength at low temperature (reversible) |
| Non-oriented electrical steel M19 elec-steel-m19 Magnetic materials | ASTM A677 fully processed, 0.35 mm | 7,650 | 200 | — | — | — | poor | 2–4 | generator stator and rotor laminations Core loss ≈ 2.4 W/kg at 1.5 T, 60 Hz |
| UHMW polyethylene uhmwpe Polymers | ASTM D4020 | 940 | 0.69 | — | 40 | — | excellent / fair ≤ 80 °C | 5–12 | wear strips, low-load bushings |
| Nylon PA66 pa66 Polymers | ASTM D4066 dry as moulded | 1,140 | 2.8 | — | 82 | — | excellent / poor ≤ 100 °C | 3–6 | gears (light duty), bushings, housings Absorbs 2.5–8 % moisture: strength and stiffness drop, dimensions grow |
| Acetal homopolymer (POM-H) pom-h Polymers | ASTM D4181 | 1,420 | 3.1 | — | 69 | — | excellent / poor ≤ 90 °C | 3–6 | small gears, cams, rollers |
| Polycarbonate (UV-stabilised) pc Polymers | ASTM D3935 | 1,200 | 2.4 | — | 65 | — | good / good ≤ 115 °C | 3–6 | covers, glazing, guards |
| ASA (weatherable) asa Polymers | ISO 6402 | 1,070 | 2.3 | — | 45 | — | excellent / excellent ≤ 85 °C | 2.5–5 | outdoor housings, covers |
| PTFE ptfe Polymers | ASTM D4894 | 2,200 | 0.5 | — | 25 | — | excellent / excellent ≤ 260 °C | 15–30 | seals, low-friction pads, bearing liners |
| EPDM rubber epdm Elastomers | ASTM D2000 AA/BA | 1,150 | — | — | 12 | — | excellent / excellent ≤ 130 °C | 3–8 | outdoor gaskets, weather seals Not oil resistant: use NBR or FKM for lubricated seals |
| Nitrile rubber (NBR) nbr Elastomers | ASTM D2000 BG | 1,000 | — | — | 14 | — | good / poor ≤ 100 °C | 3–8 | oil seals, O-rings |
| E-glass / epoxy, unidirectional (Vf ≈ 0.55) gfrp-ud-epoxy Composites | ISO 527-5 / maker data fibre direction | 2,000 | 40 | — | 1,000 | 250 | excellent / fair ≤ 80 °C | 6–15 | wind blades, spars Strongly anisotropic: transverse strength ≈ 40 MPa; fatigue to IEC 61400-23 / DNV-ST-0376 with knock-down factors |
| Carbon / epoxy, unidirectional (T300 class) cfrp-ud-epoxy Composites | ISO 527-5 / maker data fibre direction | 1,600 | 135 | — | 1,500 | 900 | excellent / fair ≤ 120 °C | 25–60 | blade spar caps, light stiff shafts Galvanic corrosion against aluminium; isolate |
| Pultruded E-glass / polyester profile gfrp-pultruded Composites | EN 13706 | 1,850 | 18 | — | 240 | — | excellent / fair ≤ 60 °C | 4–8 | VAWT blades (pultruded aerofoil), non-conductive structures |
| Douglas fir-larch No. 1 df-larch-no1 Timber | NDS Supplement (AWC) dry service | 530 | 11.7 | — | 4.7 | — | fair / fair | 1–2.5 | service platforms, temporary works NDS reference design values: Fb ≈ 6.9 MPa, Ft ≈ 4.7 MPa (adjust with NDS factors) |
| Sitka spruce (clear) sitka-spruce Timber | ASTM D143 (clear wood tests) | 400 | 10.8 | — | 70 | — | fair / poor | 4–10 | prototype blades Clear-wood values; laminated wood/epoxy blades need fatigue data |
| Concrete f'c = 28 MPa (4000 psi) concrete-28 Concrete | ACI 318 / ASTM C94 28 days | 2,400 | 24.9 | 28 | 3.3 | — | good / excellent | 0.06–0.1 | foundations, pads, piers sy holds f'c (compression); E = 4700·√f'c; modulus of rupture 0.62·√f'c; exposure class sets minimum f'c and cover (ACI 318 ch. 19–20) |
| Concrete f'c = 35 MPa (5000 psi) concrete-35 Concrete | ACI 318 / ASTM C94 28 days | 2,400 | 27.8 | 35 | 3.7 | — | good / excellent | 0.07–0.12 | foundations in freeze-thaw or sulfate exposure |
| Reinforcing bar ASTM A615 Grade 60 rebar-a615-60 Reinforcement | ASTM A615 / A706 | 7,850 | 200 | 420 | 620 | — | poor | 0.9–1.5 | foundation reinforcement Use A706 where welding or ductility is required; epoxy-coated (A775) in corrosive exposure |
| Anchor rod ASTM F1554 Grade 55 anchor-f1554-55 Carbon & alloy steels | ASTM F1554 | 7,850 | 200 | 379 | 517 | — | poor | 2–4 | tower anchor bolts Grade 55 weldable with supplement S1; hot-dip galvanise per F2329 |
| Non-shrink cementitious grout grout-c1107 Grouts | ASTM C1107 | 2,200 | — | 50 | — | — | good / excellent | 0.5–1.5 | base plate bedding f'c ≈ 35–55 MPa at 28 days per product |
| Low-iron tempered solar glass glass-low-iron Glass | EN 12150 / IEC 61215 fully tempered, 3.2 mm | 2,500 | 70 | — | 120 | — | excellent / excellent | 1.5–3 | PV module front glass, solar collector glazing Solar transmittance ≈ 91 % (≈ 94 % with AR coating) |
| Monocrystalline silicon cells (PERC/TOPCon) si-mono-perc PV cells | IEC 61215 / IEC 60904 | 2,330 | 130 | — | — | — | good ≤ 85 °C | — | PV modules Module efficiency ≈ 21–23 %; temperature coefficient ≈ −0.30 to −0.35 %/°C; NOCT ≈ 42–45 °C |
| Hot-dip galvanising coat-hdg-a123 Coatings | ASTM A123 / ISO 1461 | 7,140 | — | — | — | — | excellent / excellent | — | structural steel, anchor rods (ASTM F2329) ≈ 85 µm typical; life ≈ 50+ years in rural C2, ≈ 20 years in coastal C4 (ISO 9223) |
| Epoxy primer + polyurethane topcoat coat-epoxy-pu Coatings | ISO 12944 (C4/C5 systems) | 1,400 | — | — | — | — | good / excellent | — | towers, housings Specify ISO 12944 corrosivity category and durability class |
| Lithium-complex grease NLGI 2 grease-lic-nlgi2 Lubricants | ASTM D4950 GC-LB | 900 | — | — | — | — | good ≤ 150 °C | — | rolling bearings, main shaft bearings −30 to +150 °C; relubrication interval per bearing maker |
| Gear oil ISO VG 220 (EP, synthetic PAO) oil-iso-vg220 Lubricants | ISO 12925-1 CKD / AGMA 9005 | 860 | — | — | — | — | good ≤ 100 °C | — | enclosed gearboxes Synthetic preferred for wide temperature range and long drain intervals in wind service |
| Structural epoxy adhesive (2-part) adh-epoxy-2k Adhesives | ASTM D1002 (lap shear) | 1,300 | — | — | 25 | — | excellent / fair ≤ 80 °C | — | blade bonding, magnet retention Lap-shear ≈ 20–30 MPa on prepared aluminium; design strength far lower — test the joint |
For concrete, Sy is f'c (compressive strength). Source on every row: Typical handbook values (ASM Handbook, Shigley App. A, maker datasheets); verify against the governing specification.